Initial data:
425 cement: 320, sulpho-aluminous cement: 60, hemihydrate gypsum: 7.4
Ash calcium: 7.4, coarse whiting: 128, Sand: 463, Polycarboxylic acid: 0.6
Tartaric acid: 0.32, Glucose: 0.4, Early strength agent: 0.8
Defoaming agent: 0.8, Cellulose ether: 1.28, Redispersible polymer powder: 11.12
The initial fluidity is 133, and after 10 minutes, it is 117. The fluidity loss is a bit large (add some retarder), the water collection time is 38 minutes (it is reasonable in summer, but I am afraid it will be longer if the retarder is added), and cracks appear on the glass after ten minutes. That’s it for now; I’ll update the strength of the sample on the glass the next day.
425 cement: 320, sulpho-aluminous cement: 60, hemihydrate gypsum: 7.4
Ash calcium: 7.4, coarse whiting: 128, Sand: 463, Polycarboxylic acid: 0.6
Tartaric acid: 0.32, Glucose: 0.4, Early strength agent: 0.8
Defoaming agent: 0.8, Cellulose ether: 1.28, Redispersible polymer powder: 11.12
The initial fluidity is 133, and after 10 minutes, it is 117. The fluidity loss is a bit large (add some retarder), the water collection time is 38 minutes (it is reasonable in summer, but I am afraid it will be longer if the retarder is added), and cracks appear on the glass after ten minutes. That’s it for now; I’ll update the strength of the sample on the glass the next day.